Skip to main content

Table 3 Mixing procedure

From: Influence of functionalized S–SBR on silica–filled rubber compound properties

1st stage

Internal mixer

 Time

  0:00

Polymers

  1:20

1/2 silica, 1/2 TESPT, Oil

  2:50

1/2 silica, 1/2 TESPT, Stearic acid, Zinc oxide

  3:10

Mix (Control rotor speed up to 140 °C)

  4:10

Ram up, sweep, ram down

  6:40

Dump out

2nd stage

Two–roll mill

 0:00

1st masterbatch

 2:00

Sulfur, CBS, DPG

 7:00

Milling