Composite | UTS (MPa) Experimental | UTS (MPa) ROM | Δ (%) | E (GPa) Experimental | E (GPa) ROM | Δ (%) |
---|---|---|---|---|---|---|
Nylon-GF-12-90 | 220 ± 4 | 273 | 81 | 6.4 ± 0.1 | 8.3 | 77 |
Nylon-CF-12-90 | 249 ± 13 | 429 | 58 | 13.02 ± 0.06 | 21.24 | 61 |
Nylon-KF-12-90 | 158 ± 8 | 282 | 56 | 7.52 ± 0.07 | 10.26 | 73 |
Onyx-GF-12-90 | 212 ± 5 | 267 | 79 | 7.3 ± 0.1 | 9.3 | 78 |
Onyx-CF-12-90 | 278 ± 8 | 387 | 72 | 15.5 ± 0.3 | 21.6 | 72 |
Onyx-KF-12-90 | 161 ± 4 | 276 | 58 | 8.00 ± 0.07 | 10.99 | 73 |